The 6082 Al alloy process through cryorolling and followed by annealing.
The recovery, recrystallisation and grain growth explained through EBSD, TEM and DSC.
The recovery and recrystallisation occurs between 110 and 250 °C and 250–300 °C and beyond that grain growth started.
Cryorolled samples have excellent mechanical property after annealing at 150 °C.
Cryorolled samples annealed at 350 °C shows excellent corrosion resistance.