油酸钠体系中磁化处理对萤石浮选行为的影响
详细信息    查看全文 | 推荐本文 |
  • 英文篇名:Effect of Magnetization Treatment on Fluorite Flotation Behavior in Sodium Oleate System
  • 作者:李青青 ; 周文波 ; 李赛 ; 陶黎明 ; 余凡 ; 张力
  • 英文作者:Li Qingqing;Zhou Wenbo;Li Sai;Tao Liming;Yu Fan;Zhang Li;College of Resources and Environmental Engineering,Wuhan University of Science and Technology;The State Key Laboratory of Refractory and Metallurgy;Hubei Key Laboratory for Efficient Utilization and Agglomeration of Metallurgic Mineral Resources;
  • 关键词:萤石浮选 ; 磁化处理 ; 吸附量 ; Zeta电位
  • 英文关键词:Fluorite flotation;;Magnetized treatment;;Adsorption capacity;;Zeta potential
  • 中文刊名:JSKS
  • 英文刊名:Metal Mine
  • 机构:武汉科技大学资源与环境工程学院;省部共建耐火材料与冶金国家重点实验室;冶金矿产资源高效利用与造块湖北省重点实验室;
  • 出版日期:2019-07-15
  • 出版单位:金属矿山
  • 年:2019
  • 期:No.517
  • 基金:省部共建耐火材料与冶金国家重点实验室青年基金项目(编号:2018QN19);; 省级大学生创新项目(编号:201710488023)
  • 语种:中文;
  • 页:JSKS201907019
  • 页数:5
  • CN:07
  • ISSN:34-1055/TD
  • 分类号:113-117
摘要
为了了解油酸钠体系中磁化处理对萤石浮选行为的影响,开展了磁化油酸钠、磁化浮选用水和磁化矿浆情况下的萤石纯矿物浮选试验,并对萤石表面油酸钠的吸附量和Zeta电位进行了研究。结果表明:①在pH=8,油酸钠浓度为1.07×10~(-4)mol/L,磁场强度为200 mT,油酸钠磁化时间为10 min,水和矿浆均磁化30 min情况下的萤石纯矿物浮选试验的回收率分别为94.48%、93.07%、91.48%,相对于未磁化条件下,回收率分别提高了7.60、6.19、4.60个百分点;同时磁化处理能有效降低油酸钠的用量,且加快萤石的浮选速率,降低选别成本。②磁化油酸钠、水和矿浆均能增大萤石表面的油酸钠吸附量,磁化油酸钠后的吸附量增长最显著,其次是磁化水。磁化处理均能使萤石表面的Zeta电位发生负移,说明磁化处理促进了油酸根离子在萤石表面的吸附。③在人工混合矿浮选试验中,磁化促进了萤石的上浮,未磁化、磁化矿浆、磁化水和磁化油酸钠条件下,萤石精矿品位分别为94.57%、94.70%、94.75%、95.94%,萤石回收率分别为86.60%、89.89%、93.01%、95.35%;磁化矿浆、磁化水和磁化油酸钠相对于未磁化条件下,萤石的回收率分别提高了3.29、6.41和8.75。
        In order to understand the effect of magnetization treatment on the flotation behavior of fluorite in sodium oleate system,flotation tests of fluorite pure mineral were carried out in the case of magnetized sodium oleate,magnetized flotation water or magnetized pulp. Amount of sodium oleate adsorbed on the surface of fluorite and zeta potential were studied.The results showed that: ①In the condition of pH=8,the concentration of sodium oleate 1.07×10~(-4) mol/L and the magnetic field intensity 200 mT,the recovery rate of pure mineral flotation tests were 94.48%,93.07% and 91.48%,when the magnetization time of sodium oleate was 10 min,the magnetization time of flotation water and pulp were 30 min,respectively. The recovery rate of pure mineral flotation tests were 94.48%,93.07%,and 91.48%,respectively. Compared with unmagnetized conditions,the recovery rate increased by 7.60,6.19 and 4.60 percentage points,respectively. At the same time,the magnetization treatment can effectively reduce the usage amount of sodium oleate,accelerate the flotation rate of fluorite and reduce the cost of separation. ②All magnetized sodium oleate,water and pulp can increase the amount of sodium oleate adsorbed on the surface of fluorite. The increasing adsorption amount of magnetized sodium oleate is the most significant,followed by magnetized water. All magnetization treatment can negatively shift the zeta potential of the fluorite surface,indicating that the magnetization treatment promotes the adsorption of oleate ions on the surface of the fluorite. ③In artificial mixed mineral flotation tests,magnetization promoted the fluorite flotation. In the conditions of no magnetization,magnetized pulp,magnetized water and sodium oleate,the fluorite concentrate grade were 94.57%,94.70%,94.75% and 95.94%,respectively,the fluorite recovery rates were 86.60%,89.89%,93.01% and 95.35%,respectively. The recovery rates of fluorite using magnetized pulp,magnetized water and sodium oleate were increased by 3.29,6.41 and 8.75 percentage points,respectively,compared to unmagnetized conditions.
引文
[1]A·尤卡尔.萤石浮选中捕收剂的吸附机理[J].国外金属矿选矿,2003(7):20-23.A·Yukar.Adsorption mechanism of fluorite flotation collector[J].Metallic Ore Dressing Abroad,2003(7):20-23.
    [2]宋翔宇,赵新昌,徐会存,等.某地萤石矿浮选工艺及机理研究[J].矿冶工程,2004(3):28-31.Song Xiangyu,Zhao Xinchang,Xu Huicun,et al.Flotation separation of a certain fluorite ore and its machanism[J].Mining and Metallurgical Engineering,2004(3):28-31.
    [3]格列姆博茨基,郑飞.浮选过程物理化学基础[M].北京:冶金工业出版社,1985.Glem Botsky,Zheng Fei.Physical Chemistry Foundation of Flotation Process[M].Beijing:Metallurgical Industry Press,1985.
    [4]卢寿慈,翁达.界面分选原理及应用[M].北京:冶金工业出版社,1992.Lu Shouci,Weng Da.Principle and Application of Interface Sorting[M].Beijing:Metallurgical Industry Press,1992.
    [5]崔立凤.磁场条件下硫化铜矿浮选电化学过程及机理研究[D].赣州:江西理工大学,2009.Cui Lifeng.Study on Electrochemical Process and Mechanism of Copper Sulfide Ore Flotation Under Magnetic Field[D].Ganzhou:Jiangxi University of Technology,2009.
    [6]熊彦权,张希梅,胡炳双.煤泥磁化浮选机理的研究[J].应用能源技术,2004(4):12-14.Xiong Yanquan,Zhang Ximei,Hu Bingshuang.Study on mechanism of coal slurry magnetization flotation[J].Apply Energy Technology,2004(4):12-14.
    [7]徐秋生.磁化烃油选钼试验研究[J].金属矿山,2006(9):53-54.Xu Qiusheng.Research on magnetization hydrocarbon oil for molybdenum separation[J].Metal Mine,2006(9):53-54.
    [8]Mahmoud B,Yosra M,Nadia A.Effects of magnetic treatment on scaling power of hard waters[J].Separation&Purification Technology,2016,171:88-92.
    [9]周文波,李青青,向军,等.磁化水对萤石浮选的影响机理研究[J].非金属矿,2018(5):57-59Zhou Wenbo,Li Qingqing,Xiang Jun,et al.Study on the influence mechanism of magnetized water on fluorite flotation[J].Nonmetallic Mines,2018(5):57-59.
    [10]王有凯,魏慧男.变频磁化水对混凝土抗裂性能影响的研究[J].建筑结构,2018(22):107-111.Wang Youkai,Wei Huinan.Study on influence of frequency-converted magnetized water on crack resistance of concrete[J].Building Structure,2018(22):107-111.

© 2004-2018 中国地质图书馆版权所有 京ICP备05064691号 京公网安备11010802017129号

地址:北京市海淀区学院路29号 邮编:100083

电话:办公室:(+86 10)66554848;文献借阅、咨询服务、科技查新:66554700